Free Acids, Total Acids, Free Irons in Zinc phosphating Tanks

by Dr E. Ramanathan

📌 Zinc Phosphating – Key Parameters

  • Free Acid (FA): Unreacted phosphoric acid. Controls aggressiveness.
  • Total Acid (TA): Total acid content, includes both free and bound (complexed) acid.
  • TA/FA Ratio: Indicates bath age and buffering. Ideal around 8–12.
  • Free Iron (Fe²⁺): Accumulates with use. Should be controlled; excess inhibits coating.
  • Nitrite Accelerator: Boosts coating formation and regulates iron pick-up.

Recommended Operating Ranges – Cold & Hot Immersion Zinc Phosphating

ParameterCold ImmersionHot Immersion
Bath Temp25–40°C50–65°C
Free Acid (FA)0.8 – 1.2 points1.0 – 2.0 points
Total Acid (TA)8 – 12 points12 – 18 points
TA/FA Ratio8 – 128 – 12
Free Iron (Fe²⁺)< 0.5 g/L< 0.3 g/L
Nitrite Dose0.1 – 0.3 g/L (Sodium Nitrite)0.2 – 0.5 g/L (Sodium Nitrite)
Zinc Content1.0 – 1.5 g/L1.5 – 2.5 g/L
Coating Weight1.0 – 2.5 g/m²2.0 – 4.5 g/m²

📈 Correlations Summary

When…Then…
Free Acid too high (>2.0)Coating becomes coarse; risk of under- or over-etching
TA/FA too low (<6)Bath becomes unstable; poor coating formation
Free Iron too high (>0.5 g/L)Reduces coating weight and uniformity
Nitrite too low (<0.1 g/L)Coating is thin and patchy
Nitrite too high (>0.5 g/L)May cause over-acceleration; dusty or soft coatings

If you want more details please WhatsApp to me @ 9444929163 to fix up an appointment.

Recommended Supplier of Phosphate Coating Tank:

Leave a Reply